BULLETIN OF THE CHINESE CERAMIC SOCIETY ›› 2026, Vol. 45 ›› Issue (7): 2357-2367.DOI: 10.16552/j.cnki.issn1001-1625.2025.1179
• Solid Waste and Eco-Materials • Previous Articles Next Articles
LYU Peng1(
), LU Boyong2, QIAN Lun2, HUANG Shenye3, SONG Jiaxin3, XIE Longjie3, HUANG Wei3(
)
Received:2025-12-01
Revised:2026-02-14
Online:2026-07-15
Published:2026-08-13
Contact:
HUANG Wei
CLC Number:
LYU Peng, LU Boyong, QIAN Lun, HUANG Shenye, SONG Jiaxin, XIE Longjie, HUANG Wei. Mechanism of Mechanical and Thermal Activation to Improve Activity of Ferronickel Slag[J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2026, 45(7): 2357-2367.
| Composition | SiO2 | Al2O3 | Fe2O3 | CaO | MgO | Na2O | K2O | SO3 | TiO2 | MnO | Cr2O3 | Ni2O3 |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Mass fraction/% | 27.51 | 21.59 | 0.95 | 29.97 | 13.75 | 0.56 | 0.22 | 2.27 | 0.66 | 1.52 | 0.78 | 0.22 |
Table 1 Main chemical composition of ferronickel slag
| Composition | SiO2 | Al2O3 | Fe2O3 | CaO | MgO | Na2O | K2O | SO3 | TiO2 | MnO | Cr2O3 | Ni2O3 |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Mass fraction/% | 27.51 | 21.59 | 0.95 | 29.97 | 13.75 | 0.56 | 0.22 | 2.27 | 0.66 | 1.52 | 0.78 | 0.22 |
| Type | Size/μm | Fineness/μm | Density/(g∙cm-3) | SiO2 mass fraction/% | Fe2O3 mass fraction/% |
|---|---|---|---|---|---|
| Quartz powder | 37 | 37 | — | — | — |
Table 2 Basic property index of quartz sand
| Type | Size/μm | Fineness/μm | Density/(g∙cm-3) | SiO2 mass fraction/% | Fe2O3 mass fraction/% |
|---|---|---|---|---|---|
| Quartz powder | 37 | 37 | — | — | — |
| Sample No. | Quartz sand mass/g | Water mass/g | Mechanical activation time/min | Thermal activation temperature/℃ | |||
|---|---|---|---|---|---|---|---|
| Ferronickel slag mass/g | Slag mass/g | Cement mass/g | |||||
| S1-30% | 0 | 127.2 | 296.8 | 954 | 169.6 | 0 | — |
| C1-0% | 0 | 0 | 424.0 | 954 | 169.6 | 0 | — |
| M0-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | 0 | — |
| M1-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | 40 | — |
| M2-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | 50 | — |
| M3-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | 60 | — |
| M4-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | 70 | — |
| T0-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | — | 0 |
| T1-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | — | 400 |
| T2-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | — | 500 |
| T3-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | — | 600 |
| T4-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | — | 700 |
Table 3 Mix proportion of ferronickel slag mortar with different mechanical activation time and thermal activation temperatures
| Sample No. | Quartz sand mass/g | Water mass/g | Mechanical activation time/min | Thermal activation temperature/℃ | |||
|---|---|---|---|---|---|---|---|
| Ferronickel slag mass/g | Slag mass/g | Cement mass/g | |||||
| S1-30% | 0 | 127.2 | 296.8 | 954 | 169.6 | 0 | — |
| C1-0% | 0 | 0 | 424.0 | 954 | 169.6 | 0 | — |
| M0-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | 0 | — |
| M1-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | 40 | — |
| M2-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | 50 | — |
| M3-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | 60 | — |
| M4-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | 70 | — |
| T0-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | — | 0 |
| T1-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | — | 400 |
| T2-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | — | 500 |
| T3-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | — | 600 |
| T4-30% | 127.2 | 0 | 296.8 | 954 | 169.6 | — | 700 |
| Curing age/d | Activity index | ||||
|---|---|---|---|---|---|
| M0-30% | M1-30% | M2-30% | M3-30% | M4-30% | |
| 3 | 0.62 | 0.67 | 0.70 | 0.75 | 0.66 |
| 7 | 0.64 | 0.71 | 0.75 | 0.80 | 0.70 |
| 28 | 0.72 | 0.79 | 0.81 | 0.88 | 0.77 |
Table 4 Activity index of ferronickel slag under different mechanical activation time
| Curing age/d | Activity index | ||||
|---|---|---|---|---|---|
| M0-30% | M1-30% | M2-30% | M3-30% | M4-30% | |
| 3 | 0.62 | 0.67 | 0.70 | 0.75 | 0.66 |
| 7 | 0.64 | 0.71 | 0.75 | 0.80 | 0.70 |
| 28 | 0.72 | 0.79 | 0.81 | 0.88 | 0.77 |
| Curing age/d | Activity index | ||||
|---|---|---|---|---|---|
| T0-30% | T1-30% | T2-30% | T3-30% | T4-30% | |
| 3 | 0.61 | 0.84 | 0.88 | 0.84 | 0.77 |
| 7 | 0.63 | 0.86 | 0.92 | 0.85 | 0.81 |
| 28 | 0.73 | 0.81 | 0.93 | 0.83 | 0.80 |
Table 5 Activity index of ferronickel slag under different thermal activation temperatures
| Curing age/d | Activity index | ||||
|---|---|---|---|---|---|
| T0-30% | T1-30% | T2-30% | T3-30% | T4-30% | |
| 3 | 0.61 | 0.84 | 0.88 | 0.84 | 0.77 |
| 7 | 0.63 | 0.86 | 0.92 | 0.85 | 0.81 |
| 28 | 0.73 | 0.81 | 0.93 | 0.83 | 0.80 |
| Curing age/d | Resistance/(Ω·cm-2) | ||||||
|---|---|---|---|---|---|---|---|
| S1-30% | C1-0% | M0-30% | M1-30% | M2-30% | M3-30% | M4-30% | |
| 1 | 4.90 | 5.49 | 2.46 | 2.86 | 3.10 | 3.50 | 2.78 |
| 3 | 11.26 | 12.62 | 5.66 | 6.57 | 7.12 | 8.04 | 6.39 |
| 7 | 18.16 | 18.67 | 8.78 | 10.70 | 11.80 | 13.17 | 10.43 |
| 14 | 22.17 | 26.86 | 15.11 | 18.04 | 18.88 | 21.82 | 17.20 |
| 28 | 24.36 | 29.51 | 16.60 | 19.82 | 20.74 | 23.97 | 18.90 |
Table 6 Resistance of ferronickel slag mortar under different mechanical activation time
| Curing age/d | Resistance/(Ω·cm-2) | ||||||
|---|---|---|---|---|---|---|---|
| S1-30% | C1-0% | M0-30% | M1-30% | M2-30% | M3-30% | M4-30% | |
| 1 | 4.90 | 5.49 | 2.46 | 2.86 | 3.10 | 3.50 | 2.78 |
| 3 | 11.26 | 12.62 | 5.66 | 6.57 | 7.12 | 8.04 | 6.39 |
| 7 | 18.16 | 18.67 | 8.78 | 10.70 | 11.80 | 13.17 | 10.43 |
| 14 | 22.17 | 26.86 | 15.11 | 18.04 | 18.88 | 21.82 | 17.20 |
| 28 | 24.36 | 29.51 | 16.60 | 19.82 | 20.74 | 23.97 | 18.90 |
| Curing age/d | Resistance/(Ω·cm-2) | ||||||
|---|---|---|---|---|---|---|---|
| S1-30% | C1-0% | T0-30% | T1-30% | T2-30% | T3-30% | T4-30% | |
| 1 | 4.94 | 5.53 | 2.42 | 4.25 | 4.57 | 4.03 | 3.69 |
| 3 | 11.36 | 12.72 | 5.58 | 9.78 | 10.51 | 9.18 | 8.50 |
| 7 | 18.30 | 18.81 | 8.65 | 14.96 | 16.60 | 14.68 | 13.59 |
| 14 | 21.96 | 26.65 | 15.32 | 18.67 | 20.70 | 19.51 | 18.25 |
| 28 | 24.13 | 29.28 | 16.83 | 20.51 | 23.04 | 21.44 | 20.05 |
Table 7 Resistance of ferronickel slag mortar under different thermal activation temperatures
| Curing age/d | Resistance/(Ω·cm-2) | ||||||
|---|---|---|---|---|---|---|---|
| S1-30% | C1-0% | T0-30% | T1-30% | T2-30% | T3-30% | T4-30% | |
| 1 | 4.94 | 5.53 | 2.42 | 4.25 | 4.57 | 4.03 | 3.69 |
| 3 | 11.36 | 12.72 | 5.58 | 9.78 | 10.51 | 9.18 | 8.50 |
| 7 | 18.30 | 18.81 | 8.65 | 14.96 | 16.60 | 14.68 | 13.59 |
| 14 | 21.96 | 26.65 | 15.32 | 18.67 | 20.70 | 19.51 | 18.25 |
| 28 | 24.13 | 29.28 | 16.83 | 20.51 | 23.04 | 21.44 | 20.05 |
| [1] | 李小明, 沈苗, 王翀, 等. 镍渣资源化利用现状及发展趋势分析[J]. 材料导报, 2017, 31(5): 100-105. |
| LI X M, SHEN M, WANG C, et al. Current situation and development of comprehensive utilization of nickel slag[J]. Materials Review, 2017, 31(5): 100-105 (in Chinese). | |
| [2] |
WANG D Q, MA B, PANG L, et al. Alkali-activated blast furnace ferronickel slag for Cr immobilization[J]. Cement and Concrete Composites, 2024, 150: 105560.
DOI URL |
| [3] |
WANG W L, CHEN J Y, YU J, et al. Adjusting the melting and crystallization behaviors of ferronickel slag via partially replacing of SiO2 by B2O3 for mineral wool production[J]. Waste Management, 2020, 111: 34-40.
DOI URL |
| [4] |
HUANG Y D, WANG Q, SHI M X. Characteristics and reactivity of ferronickel slag powder[J]. Construction and Building Materials, 2017, 156: 773-789.
DOI URL |
| [5] |
ZHOU Y Q, SHI C F. Experimental study of electric furnace ferronickel slag as a supplementary cementitious material in massive high-strength concrete[J]. Journal of Thermal Analysis and Calorimetry, 2022, 147(8): 4983-4993.
DOI |
| [6] |
WANG Y B, HE X Y, SU Y, et al. Efficiency of wet-grinding on the mechano-chemical activation of granulated blast furnace slag (GBFS)[J]. Construction and Building Materials, 2019, 199: 185-193.
DOI URL |
| [7] |
ZHU H J, MA M Y, HE X Y, et al. Effect of wet-grinding steel slag on the properties of Portland cement: an activated method and rheology analysis[J]. Construction and Building Materials, 2021, 286: 122823.
DOI URL |
| [8] |
TAN H B, LI M G, HE X Y, et al. Effect of wet grinded lithium slag on compressive strength and hydration of sulphoaluminate cement system[J]. Construction and Building Materials, 2021, 267: 120465.
DOI URL |
| [9] |
ZHU S, HU J G, ZHANG C H, et al. Study on optimization and mechanism of mechanical activation process of titanium-bearing blast furnace slag[J]. Journal of Materials Research and Technology, 2022, 19: 3130-3144.
DOI URL |
| [10] | 张 涛, 陈铁军, 潘料庭, 等. 机械活化和不锈钢渣掺量对矿渣胶凝材料性能的影响[J]. 硅酸盐通报, 2022, 41(2): 553-561. |
| ZHANG T, CHEN T J, PAN L T, et al. Effects of mechanical activation and stainless steel slag content on the properties of slag cementitious materials[J]. Bulletin of the Chinese Ceramic Society, 2022, 41(2): 553-561 (in Chinese). | |
| [11] |
WANG Y R, WANG D M, ZHENG Y, et al. Thermal activation mechanism and activity evaluation of lithium slag: insights from simulated hydration[J]. Construction and Building Materials, 2024, 411: 134615.
DOI URL |
| [12] |
LI Y, TANG X, ZHAO H Z, et al. Influence of calcination temperature on steel slag activity for preparing a gel material[J]. Journal of Iron and Steel Research International, 2025, 32: 1-13.
DOI |
| [13] |
RAMANATHAN S, KASANIYA M, TUEN M, et al. Linking reactivity test outputs to properties of cementitious pastes made with supplementary cementitious materials[J]. Cement and Concrete Composites, 2020, 114: 103742.
DOI URL |
| [14] |
KANG S X, WANG J Z, HU C, et al. The influence of mechanochemical activation on the rheological properties and strength development of geopolymer[J]. Journal of Building Engineering, 2024, 96: 110585.
DOI URL |
| [15] |
ZERZOURI M, HAMZAOUI R, ZIYANI L, et al. Influence of slag based pre-geopolymer powders obtained by mechanosynthesis on structure, microstructure and mechanical performance of geopolymer pastes[J]. Construction and Building Materials, 2022, 361: 129637.
DOI URL |
| [16] |
MINO L, SPOTO G, BORDIGA S, et al. Particles morphology and surface properties as investigated by HRTEM, FTIR, and periodic DFT calculations: from pyrogenic TiO2 (P25) to nanoanatase[J]. The Journal of Physical Chemistry C, 2012, 116(32): 17008-17018.
DOI URL |
| [17] |
REAL S, CARRICO A, BOGAS J A, et al. Influence of the treatment temperature on the microstructure and hydration behavior of thermoactivated recycled cement[J]. Materials, 2020, 13(18): 3937.
DOI URL |
| [18] |
DJOBO J N Y, ELIMBI A, TCHAKOUTÉ H K, et al. Mechanical activation of volcanic ash for geopolymer synthesis: effect on reaction kinetics, gel characteristics, physical and mechanical properties[J]. RSC Advances, 2016, 6(45): 39106-39117.
DOI URL |
| [19] |
KUMAR R, KUMAR S, BADJENA S, et al. Hydration of mechanically activated granulated blast furnace slag[J]. Metallurgical and Materials Transactions B, 2005, 36(6): 873-883.
DOI URL |
| [20] |
ZHANG X Z, ZHANG Z Y, ZHOU J B, et al. Thermal behavior and mechanism study of geopolymers prepared from ferronickel slag with high fire resistance[J]. Construction and Building Materials, 2024, 438: 137282.
DOI URL |
| [21] |
LUO Y, LI S H, KLIMA K M, et al. Degradation mechanism of hybrid fly ash/slag based geopolymers exposed to elevated temperatures[J]. Cement and Concrete Research, 2022, 151: 106649.
DOI URL |
| [22] |
KALINA R D, AL-SHMAISANI S, FERRON R D, et al. False positives in ASTM C618 specifications for natural pozzolans[J]. ACI Materials Journal, 2019, 116(1): 165-172.
DOI |
| [23] |
HUANG W, HE L, CHEN Z D, et al. Effect of endogenous chloride ion on the corrosion behavior of reinforcement embedded in sea-sand UHPC matrix in different immersion environments[J]. Journal of Building Engineering, 2024, 90: 109376.
DOI URL |
| [1] | LIAO Yuntian, PENG Wenjie, LI Bo, CHEN Wei, ZHENG Xuhang. Effect of Activation Process on Properties of Kaolin-Based Low-Carbon Cement [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2026, 45(6): 1979-1987. |
| [2] | WANG Wei, YE Zi, YU Qi, ZHANG Yamei. Influence of Initial Particle Size of Ferronickel Slag on Alkali-Silica Reaction in Cement Mortar [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2026, 45(4): 1109-1121. |
| [3] | CUI Yingbin, LIAN Haikun, LIU Fangfang, WANG Zhen, FAN Taotao, SI Chundi, LI Zixuan. Optimization Methods and Activation Mechanisms for Enhancing Activity of Coal Gangue Powder [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2026, 45(2): 528-539. |
| [4] | QIU Junfu, ZHANG Ruifeng, HE Xinxin, ZHAO Yuxiang, HU Jialei, LI Yaxi. Mechanism Study on Influences of Heat Treatment Temperature and Storage Time on Activity of Construction Waste Separation Residue [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2025, 44(9): 3355-3366. |
| [5] | YANG Kailu, YANG Dingyi, LU Shimin, CHEN Longxiang, MAO Xiang, ZHAO Jian. Comparison and Optimization of Metakaolin Activity Determination Methods [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2025, 44(7): 2514-2527. |
| [6] | LI Jianhua, DENG Qiang, ZHAO Zhongjun, JIA Xiangyang, TANG Guowang, ZHOU Kai, FANG Kuizhen, YUAN Huikai. Influence of Low-Calcium Fly Ash Vitreous Content on Strength Development [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2025, 44(6): 2201-2209. |
| [7] | MA Shaolin, MING Yang, LI Wenjun, REN Hao, LIU Yongdao, TIAN Wei, ZHANG Guozhi, CHEN Feixiang, DOU Guangyuan, FAN Zhihong. Preparation and Performance of Ultrafine and High Active Mineral Admixture by Multiple Solid Wastes Synergy [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2025, 44(5): 1824-1833. |
| [8] | ZHANG Xiuze, HUANG Min, HUANG Muyang, LI Mengke, GE Chuyi, LIAO Xianqing, BAO Shenxu. Preparation and Mechanism of Thermal Activation Shield Muck-Based Ceramsite [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2025, 44(4): 1556-1565. |
| [9] | QIU Xiumei, LIU Yi, LIU Yadong, CAI Hao, LIU Yedongyang, LIANG Yaqi. Green Preparation of Self-Forming Type A Zeolite Foam from Activated Rectorite [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2025, 44(12): 4623-4632. |
| [10] | NING Gaopeng, ZHOU Zhengyuan, XIA Guanghua, WU Wenxing, CAO Tianyi, CHEN Yushan. Effects of Sintering Temperature and Mechanically Activated Time on Ceramic Tiles Preparation with Ceramic Solid Waste [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2024, 43(8): 3026-3033. |
| [11] | HU Kaiwei, CHEN Xuan, LI Tingfeng, ZHANG Junjie, GAO Xuan, YANG Tao. Effect of Mechanical Activation on Early-Age Performance of Sodium Carbonate-Activated GBFS Binders [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2024, 43(7): 2577-2583. |
| [12] | WU Yuanting, WANG Yuanchen, WANG Zhao, LIU Hulin, WANG Wei, REN Siqian, HUA Chunfeng. Effect of Organic Ethanolamine TEA-M-Inorganic Salt System on Activation of FBC [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2024, 43(2): 572-583. |
| [13] | WANG Wenyao, LUO Qi, LU Liulei, LAI Jin, HUANG Wenhao, ZHUANG Rongchuan, WANG Junfeng, MA Jun. Preparation and Properties of Sulfur Tailings-Based Geopolymer Activated by Alkaline Hydrothermal Method [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2024, 43(10): 3704-3714. |
| [14] | ZHU Pengfei, YU Yi, SHI Yanran, YANG Heng, HE Yang, XU Fei, JIANG Linhua, CHU Hongqiang, XU Tianlei, XU Ning. Pore Structure Evolution of Limestone Powder Hardened Cement Slurry Based on Electrochemical Impedance Spectroscopy [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2024, 43(1): 35-43. |
| [15] | CHEN Libao, LIU Guangyan, JIN Linsen, MU Song, WANG Tao, TANG Jinhui. Protective Behavior of Zinc Sacrificial Anode on Steel Bars under Carbonization and Chloride Salt Erosion [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2024, 43(1): 113-120. |
| Viewed | ||||||
|
Full text |
|
|||||
|
Abstract |
|
|||||