BULLETIN OF THE CHINESE CERAMIC SOCIETY ›› 2026, Vol. 45 ›› Issue (2): 471-481.DOI: 10.16552/j.cnki.issn1001-1625.2025.0873
• Cement and Concrete • Previous Articles Next Articles
GUO Yongmin1(
), ZHANG Longjiao1, AN Xinzheng2(
), LI Weizhi3, AN Shuhao1, JI Mengqi1, WANG Yan1
Received:2025-08-29
Revised:2025-10-04
Online:2026-02-20
Published:2026-03-09
Contact:
AN Xinzheng
CLC Number:
GUO Yongmin, ZHANG Longjiao, AN Xinzheng, LI Weizhi, AN Shuhao, JI Mengqi, WANG Yan. Acoustic Emission Parameter Calibration and Source Localization Accuracy in Steel Fiber Reinforced Concrete[J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2026, 45(2): 471-481.
| Aggregate type | Porosity/% | Fragmentation index/% | Apparent density/(kg⋅m-3) | Bulk density/(kg⋅m-3) |
|---|---|---|---|---|
| Crushed stone | 13.2 | 11.7 | 2 647 | 1 575 |
Table 1 Physical properties of coarse aggregate
| Aggregate type | Porosity/% | Fragmentation index/% | Apparent density/(kg⋅m-3) | Bulk density/(kg⋅m-3) |
|---|---|---|---|---|
| Crushed stone | 13.2 | 11.7 | 2 647 | 1 575 |
| Fiber type | Fiber length/mm | Equivalent diameter/mm | Aspect ratio/mm | Tensile strength/MPa |
|---|---|---|---|---|
| End-hook type | 25 | 0.83 | 30 | ≥600 |
| Shear type | 35 | 0.85 | 40 | ≥600 |
| Corrugated type | 38 | 1.11 | 34 | ≥600 |
Table 2 Major properties of steel fiber
| Fiber type | Fiber length/mm | Equivalent diameter/mm | Aspect ratio/mm | Tensile strength/MPa |
|---|---|---|---|---|
| End-hook type | 25 | 0.83 | 30 | ≥600 |
| Shear type | 35 | 0.85 | 40 | ≥600 |
| Corrugated type | 38 | 1.11 | 34 | ≥600 |
| Specimen | Lead break angle/(°) | Sensor 1 amplitude/dB | Standard deviation | Sensor 2 amplitude/dB | Standard deviation |
|---|---|---|---|---|---|
| T1 | 15 | 40.7 | 0.69 | 39.8 | 0.72 |
| 30 | 41.2 | 1.42 | 40.4 | 1.58 | |
| 60 | 41.8 | 0.83 | 40.1 | 1.23 | |
| T2 | 15 | 42.5 | 1.55 | 41.6 | 0.91 |
| 30 | 40.4 | 2.02 | 39.4 | 1.11 | |
| 60 | 41.7 | 1.54 | 39.9 | 1.53 | |
| T3 | 15 | 43.1 | 1.63 | 41.2 | 0.56 |
| 30 | 43.5 | 1.98 | 40.9 | 0.93 | |
| 60 | 42.3 | 0.75 | 42.1 | 0.42 | |
| T4 | 15 | 40.9 | 0.63 | 38.7 | 0.78 |
| 30 | 42.6 | 1.11 | 40.5 | 0.86 | |
| 60 | 41.3 | 0.96 | 40.7 | 0.85 |
Table 3 AE signal amplitudes of different specimens
| Specimen | Lead break angle/(°) | Sensor 1 amplitude/dB | Standard deviation | Sensor 2 amplitude/dB | Standard deviation |
|---|---|---|---|---|---|
| T1 | 15 | 40.7 | 0.69 | 39.8 | 0.72 |
| 30 | 41.2 | 1.42 | 40.4 | 1.58 | |
| 60 | 41.8 | 0.83 | 40.1 | 1.23 | |
| T2 | 15 | 42.5 | 1.55 | 41.6 | 0.91 |
| 30 | 40.4 | 2.02 | 39.4 | 1.11 | |
| 60 | 41.7 | 1.54 | 39.9 | 1.53 | |
| T3 | 15 | 43.1 | 1.63 | 41.2 | 0.56 |
| 30 | 43.5 | 1.98 | 40.9 | 0.93 | |
| 60 | 42.3 | 0.75 | 42.1 | 0.42 | |
| T4 | 15 | 40.9 | 0.63 | 38.7 | 0.78 |
| 30 | 42.6 | 1.11 | 40.5 | 0.86 | |
| 60 | 41.3 | 0.96 | 40.7 | 0.85 |
| Steel fiber content/% | Average sound velocity/(m·s-1) | Standard deviation | Coefficient of variation(C.V.)/% |
|---|---|---|---|
| 0 | 3 595.44 | 24.32 | 0.68 |
| 0.5 | 3 449.80 | 78.43 | 2.27 |
| 1.0 | 3 359.70 | 97.46 | 2.90 |
| 1.5 | 3 261.14 | 111.96 | 3.54 |
Table 4 Descriptive statistics on effect of steel fiber content on sound velocity
| Steel fiber content/% | Average sound velocity/(m·s-1) | Standard deviation | Coefficient of variation(C.V.)/% |
|---|---|---|---|
| 0 | 3 595.44 | 24.32 | 0.68 |
| 0.5 | 3 449.80 | 78.43 | 2.27 |
| 1.0 | 3 359.70 | 97.46 | 2.90 |
| 1.5 | 3 261.14 | 111.96 | 3.54 |
| Source of mutation | Sum of squares (SS) | degree of freedom (df) | Mean square (MS) | F-value | Significance (P) |
|---|---|---|---|---|---|
| Between groups (BG) | 649 488.9 | 3 | 216 496.3 | 32.89 | <0.001 |
| Within groups (WG) | 184 084.1 | 28 | 6 574.43 | ||
| Total (T) | 833 573.0 | 31 |
Table 5 Single factor analysis results of variance on effect of steel fiber content on sound velocity
| Source of mutation | Sum of squares (SS) | degree of freedom (df) | Mean square (MS) | F-value | Significance (P) |
|---|---|---|---|---|---|
| Between groups (BG) | 649 488.9 | 3 | 216 496.3 | 32.89 | <0.001 |
| Within groups (WG) | 184 084.1 | 28 | 6 574.43 | ||
| Total (T) | 833 573.0 | 31 |
| Group (I) | Group (J) | Mean difference/(m·s-1) | P-value | Significance (P<0.05) |
|---|---|---|---|---|
| 0% | 0.5% | 145.64 | <0.001 | Yes |
| 0% | 1.0% | 235.74 | <0.001 | Yes |
| 0% | 1.5% | 434.30 | <0.001 | Yes |
| 0.5% | 1.0% | 90.10 | <0.001 | Yes |
| 0.5% | 1.5% | 288.66 | <0.001 | Yes |
| 1.0% | 1.5% | 198.56 | <0.001 | Yes |
Table 6 Tukey’s post hoc test results for multiple comparisons of mean sound velocity
| Group (I) | Group (J) | Mean difference/(m·s-1) | P-value | Significance (P<0.05) |
|---|---|---|---|---|
| 0% | 0.5% | 145.64 | <0.001 | Yes |
| 0% | 1.0% | 235.74 | <0.001 | Yes |
| 0% | 1.5% | 434.30 | <0.001 | Yes |
| 0.5% | 1.0% | 90.10 | <0.001 | Yes |
| 0.5% | 1.5% | 288.66 | <0.001 | Yes |
| 1.0% | 1.5% | 198.56 | <0.001 | Yes |
| Parameter | Threshold/dB | Sound velocity/(m·s-1) | PDT/μs | HDT/μs | HLT/μs |
|---|---|---|---|---|---|
| Value | 40 | 3 507 | 150 | 300 | 500 |
Table 7 Values of parameters related to AE
| Parameter | Threshold/dB | Sound velocity/(m·s-1) | PDT/μs | HDT/μs | HLT/μs |
|---|---|---|---|---|---|
| Value | 40 | 3 507 | 150 | 300 | 500 |
| [1] |
RADOJIČIĆ V, RADULOVIĆ R, TARIĆ M, et al. The influence of the steel fibers on improvement of mechanical characteristic of concrete[J]. Mechanics Based Design of Structures and Machines, 2022, 50(8): 2929-2939.
DOI URL |
| [2] |
SHI X J, PARK P, REW Y, et al. Constitutive behaviors of steel fiber reinforced concrete under uniaxial compression and tension[J]. Construction and Building Materials, 2020, 233: 117316.
DOI URL |
| [3] | MU R, WEI L S, WANG X W, et al. Preparation of aligned steel fiber reinforced cementitious composite and its flexural behavior[J]. Journal of Visualized Experiments, 2018(136): 56307. |
| [4] |
BRANSTON J, DAS S, KENNO S Y, et al. Mechanical behaviour of basalt fibre reinforced concrete[J]. Construction and Building Materials, 2016, 124: 878-886.
DOI URL |
| [5] |
LEE M K, BARR B I G. An overview of the fatigue behaviour of plain and fibre reinforced concrete[J]. Cement and Concrete Composites, 2004, 26(4): 299-305.
DOI URL |
| [6] |
BEHNIA A, CHAI H K, RANJBAR N, et al. Damage detection of SFRC concrete beams subjected to pure torsion by integrating acoustic emission and Weibull damage function[J]. Structural Control and Health Monitoring, 2016, 23(1): 51-68.
DOI URL |
| [7] |
LI B, XU L H, CHI Y, et al. Experimental investigation on the stress-strain behavior of steel fiber reinforced concrete subjected to uniaxial cyclic compression[J]. Construction and Building Materials, 2017, 140: 109-118.
DOI URL |
| [8] |
CHISARI C, GUARNACCIA C, RIZZANO G. Numerical simulation of acoustic emission activity in reinforced concrete structures by means of finite element modelling at the macroscale[J]. Structural Health Monitoring, 2020, 19(2): 537-551.
DOI URL |
| [9] |
SHIOTANI T. Evaluation of long-term stability for rock slope by means of acoustic emission technique[J]. NDT & E International, 2006, 39(3): 217-228.
DOI URL |
| [10] |
AGGELIS D G, MPALASKAS A C, MATIKAS T E. Investigation of different fracture modes in cement-based materials by acoustic emission[J]. Cement and Concrete Research, 2013, 48: 1-8.
DOI URL |
| [11] |
VERSTRYNGE E, VAN STEEN C, VANDECRUYS E, et al. Steel corrosion damage monitoring in reinforced concrete structures with the acoustic emission technique: a review[J]. Construction and Building Materials, 2022, 349: 128732.
DOI URL |
| [12] |
SHARMA G, SHARMA S, SHARMA S K. Fracture monitoring of steel and GFRP reinforced concrete beams using acoustic emission and digital image correlation techniques[J]. Structural Concrete, 2021, 22(4): 1962-1976.
DOI URL |
| [13] |
ZHANG H, LIU X Y, BAI L Y, et al. Acoustic emissions evaluation of the dynamic splitting tensile properties of steel fiber reinforced concrete under freeze-thaw cycling[J]. Frontiers of Structural and Civil Engineering, 2023, 17(9): 1341-1356.
DOI |
| [14] | OHTSU M. Progress in acoustic emission analysis for fracture mechanism in composite materials[J]. Cement and Concrete Research, 2023, 174: 107317. |
| [15] | ASHRAF S, RUCKA M. Comparative study on fracture evolution in steel fibre and bar reinforced concrete beams using acoustic emission and digital image correlation techniques[J]. Case Studies in Construction Materials, 2024, 20: e03359. |
| [16] |
NIE Q P, LIU H N, MA T F, et al. Experimental study on acoustic emission of steel fiber broken pebble recycled concrete[J]. Construction and Building Materials, 2024, 452: 138942.
DOI URL |
| [17] | 刘洋, 张亚梅, 侯心宇, 等. 钢纤维混凝土剪切损伤演化的声发射特性研究[J]. 土木工程学报, 2023, 56(增刊2): 374-380. |
| LIU Y, ZHANG Y M, HOU X Y, et al. Study on acoustic emission characteristics of shear damage evolution in steel fiber reinforced concrete[J]. Chinese Journal of Civil Engineering, 2023, 56(supplement 2): 374-380 (in Chinese). | |
| [18] |
BARBOSH M, LI B Q, SADHU A. Improved acoustic source localization method for crack identification in structures[J]. Applied Acoustics, 2024, 223: 110093.
DOI URL |
| [19] |
CHEN Z H, MIAO T J, LIU T, et al. Active-passive joint acoustic emission monitoring test considering the heterogeneity of concrete[J]. Materials, 2023, 16(24): 7694.
DOI URL |
| [20] | LIU T, FENG J, WANG Z, et al. Acoustic emission source localization in concrete structures using deep learning[J]. Structural Health Monitoring, 2022, 21(5): 2341-2356. |
| [21] | 陈建峰, 王子健, 王瑞芳, 等. 基于改进粒子群算法的混凝土声发射源高精度定位方法[J]. 硅酸盐学报, 2022, 50(1): 185-194. |
| CHEN J F, WANG Z J, WANG R F, et al. High-precision localization method for concrete acoustic emission sources based on an improved particle swarm optimization algorithm[J]. Journal of the Chinese Ceramic Society, 2022, 50(1): 185-194 (in Chinese). | |
| [22] |
HASSAN F, MAHMOOD A K B, YAHYA N, et al. State-of-the-art review on the acoustic emission source localization techniques[J]. IEEE Access, 2021, 9: 101246-101266.
DOI URL |
| [23] | 中国工程建设标准化协会. 纤维混凝土试验方法标准:CECS 13—2009[S]. 北京: 中国计划出版社, 2010. |
| China Association for Engineering Construction Standardization. Standard test methods for fiber reinforced concrete:CECS 13—2009[S]. Beijing: China Planning Press, 2010 (in Chinese). | |
| [24] | 戴金辉, 袁靖. 单因素方差分析与多元线性回归分析检验方法的比较[J]. 统计与决策, 2016(9): 23-26. |
| DAI J H, YUAN J. Comparison of single-factor analysis of variance and multiple linear regression analysis methods[J]. Statistics and Decision Making, 2016(9): 23-26 (in Chinese). | |
| [25] | BANKIR S, MURAT B. Experimental investigation and statistical evaluation of the effects of steel fiber aspect ratio and fiber rate on static and dynamic mechanical properties of concrete[J]. Construction and Building Materials, 2024, 414: 116790. |
| [26] |
CHEN X L, WU Z, WANG H, et al. Statistical analysis and multi-objective optimization of the chloride ion penetration resistance of recycled aggregate concrete[J]. Cement and Concrete Composites, 2023, 137: 104928.
DOI URL |
| [27] | 中华人民共和国住房和城乡建设部, 国家市场监督管理总局. 混凝土物理力学性能试验方法标准:GB/T 50081—2019[S]. 北京: 中国建筑工业出版社, 2019. |
| Ministry of Housing and Urban-Rural Development of the People’s Republic of China, State Administration for Market Regulation. Standard for test methods of concrete physical and mechanical properties: GB/T 50081—2019[S]. Beijing: China Architecture & Building Press, 2019 (in Chinese). |
| [1] | LI Xiaopeng, ZHAO Jun, CHEN Zhehan, LIANG Mengyang. Shrinkage and Prediction Model of High-Performance Micro-Fine Steel Fiber Reinforced Sulphoaluminate Cement Concrete [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2026, 45(2): 461-470. |
| [2] | WANG Qiang, WANG Jiacheng, WANG Nan, ZHANG Wei, XU Dongyu. Compressive Failure Mechanics and Acoustic Emission Characteristics of Fiber Reinforced Concrete afterHigh Temperature [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2025, 44(3): 915-923. |
| [3] | ZHU Guiwang, QIN Lei, DING Weijian, LI Pingfeng, SUN Ming. Influences of Metamaterials on Bending Toughness of Cement-Based Materials Based on Acoustic Emission Parameters [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2025, 44(2): 424-433. |
| [4] | GONG Linling, CHEN Bo, ZHOU Chengtao. Acoustic Emission Signal Recognition of Freeze-Thaw Damage Type of Foam Concrete Based on GMM-SVM [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2025, 44(10): 3620-3633. |
| [5] | WANG Xueqing, LI Yongchao, ZHANG Xuerui, ZHAO Yunmeng, JIANG Yufeng. Crack Propagation and Damage Evolution in Polypropylene Fiber Reinforced Concrete with Cracks under Axis Compression [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2024, 43(7): 2404-2414. |
| [6] | PAN Xiaofeng, CAO Jiantao, LUO Tao, TANG Liyun. Failure Precursory Characteristics of Early-Age Steel Fiber Reinforced Concrete under Uniaxial Compression [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2024, 43(7): 2470-2478. |
| [7] | ZHANG Yanbo, ZHANG Lei, HOU Ning, HUANG Feng. Acoustic Emission Characteristics and Failure Modes of Casing Material under Pulse Gas Splitting [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2024, 43(11): 3986-3995. |
| [8] | JIN Ziheng, XIE Faxiang, CAI Dingpeng, HAN Xu, ZHANG Yun. Acoustic Emission Properties of Fracture Process of Internally Cured Concrete with Super Absorbent Polymer [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2023, 42(7): 2419-2428. |
| [9] | LEI Longjian, HAO Yong, YUAN Man, DU Guofeng, YUAN Hongqiang, ZUO Qingjun. Study on Compressive Mechanical Properties of Carbon Nanotube Cement-Based Materials Based on Acoustic Emission and DIC [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2023, 42(12): 4233-4241. |
| [10] | TAO Xuejun, LUO Jianlin, FAN Kangxin, CHEN Jie, ZHU Min, GAO Yibo. Meso-Compressive Fracture Simulation and Performance Analysis of Steel Fiber Reinforced Concrete [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2023, 42(11): 3884-3894. |
| [11] | ZENG Zhiwei, LIANG Jian, ZENG Yuxin, YU Bo. Analysis of Acoustic Emission Characteristic Parameters During Whole Damage Process of Concrete under Uniaxial and Eccentric Compressions [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2022, 41(5): 1599-1608. |
| [12] | WANG Huiming, LI Rufei, DENG Pinggui. Damage and Failure Mechanism of Steel Fiber Reinforced Concrete Based on Fractal Theory and Extended Finite Element Method [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2022, 41(12): 4202-4213. |
| [13] | YANG Xiaohua, LUO Tao, LIU Xiaojian, YE Ermulati. Effect of Initial Notch-to-Depth Ratio on Fracture Properties of Steel Fiber Reinforced Concrete [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2022, 41(10): 3465-3474. |
| [14] | ZHAO Xiaohong, SHEN Yu, LIU Juanhong, GUO Zidong. Influence of Sulfate on Mechanical Properties of Shaft Wall Concrete in Ultra-Deep Wells and Its Degradation Mechanism [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2021, 40(9): 2939-2947. |
| [15] | HE Zhengbo, WANG Huiming. Fatigue Performance Analysis of Steel Fiber Reinforced Concrete Beams Combined with Homogenization Theory [J]. BULLETIN OF THE CHINESE CERAMIC SOCIETY, 2021, 40(8): 2574-2583. |
| Viewed | ||||||
|
Full text |
|
|||||
|
Abstract |
|
|||||