欢迎访问《硅酸盐通报》官方网站,今天是
分享到:

硅酸盐通报 ›› 2021, Vol. 40 ›› Issue (3): 1016-1021.

• 新型功能材料 • 上一篇    下一篇

硼标记压裂裂缝示踪剂的制备及性能

李向辉1, 遆永周1, 李灿然1, 张锋2, 陈前2, 王晓慧1, 苑素华1, 朱玉坤3   

  1. 1.河南省科学院同位素研究所有限责任公司,郑州市同位素示踪与探测重点实验室,郑州 450015;
    2.中国石油大学(华东)地球物理与信息学院,青岛 266580;
    3.河南省同新科技有限责任公司,郑州 450015
  • 收稿日期:2020-10-19 修回日期:2020-12-03 出版日期:2021-03-15 发布日期:2021-04-13
  • 通讯作者: 李灿然,助理研究员。E-mail:lcanran@163.com
  • 作者简介:李向辉(1979—),男,博士,高工。主要从事无机材料合成及同位素示踪应用研究。E-mail:lixianghuiboy@163.com
  • 基金资助:
    河南省科学院科研开发专项基本科研业务费项目(200604032,200604116);国家自然科学基金(41574119)

Preparation and Performance of Boron-Labeled Fracturing Fracture Tracer

LI Xianghui1, TI Yongzhou1, LI Canran1, ZHANG Feng2, CHEN Qian2, WANG Xiaohui1, YUAN Suhua1, ZHU Yukun3   

  1. 1. Zhengzhou Key Laboratory of Isotope Tracing and Detecting, Isotope Research Institute of Henan Academy of Sciences Co., Ltd, Zhengzhou 450015, China;
    2. College of Geophysics and Information Engineering, China University of Petroleum, Qingdao 266580, China;
    3. Henan Tongxin Technology Co., Ltd., Zhengzhou 450015, China
  • Received:2020-10-19 Revised:2020-12-03 Online:2021-03-15 Published:2021-04-13

摘要: 硼具有高的热中子捕获截面,可用于油气井下压裂裂缝的探测。通过热重分析-差热分析法(TG-DTA)、X射线衍射分析(XRD)、能谱分析(EDS)、扫描电镜(SEM)和电感耦合原子发射光谱(ICP-AES)测试方法,研究了碳化硼(B4C)不同外加量(质量分数分别为1%、5%和10%)对压裂示踪支撑剂结构和性能的影响。结果表明,当B4C外加量1%时,主晶相为刚玉相,69 MPa闭合压力下支撑剂的破碎率和体积密度分别为5.4%和1.66 g·cm-3。B4C外加量为5%和10%时,B4C氧化生成的氧化硼与氧化铝反应生成硼酸铝晶须,刚玉相减少。B4C氧化生成的二氧化碳和氧化硼的挥发,形成支撑剂的多孔结构,导致支撑剂破碎率升高和体密度下降。

关键词: 碳化硼, 压裂支撑剂, 压裂裂缝, 同位素标记, 破碎率

Abstract: Boron with high thermal neutron capture cross section can be used to detect fracturing fractures in oil and gas downhole. The effects of different amounts of B4C (mass fraction of 1%, 5%, and 10%, respectively) on the structure and performance of the fracturing proppant were investigated by thermogravimetric-differential thermal analysis (TG-DTA), X-ray diffraction analysis (XRD), energy spectrum analysis (EDS), scanning electron microscope (SEM) and inductively coupled atomic emission spectroscopy (ICP-AES). The results show that when the adding amount of B4C is 1%, its main phase is corundum. The breakage ratio and volume density under the 69 MPa pressure are 5.4% and 1.66 g·cm-3, respectively. When the B4C adding amount of is at 5% or 10%, the boron oxide generated by oxidation of B4C reacts with alumina to form aluminum borate whiskers, and the corundum phase is reduced. Carbon dioxide and boron oxide from the oxidation of B4C evaporated, form a porous structure of the proppant, and result in an increase of the breakage ratio and a decrease in bulk density.

Key words: B4C, fracturing proppant, fracturing fracture, isotope labeling, breakage ratio